u'amea nikeli Eletise tusita'i ENiCrFe-9 U'umea fai
VAEGA KEMIMI:
ALOY(wt%) | C | Mn | Si | Fe | Cr | Ni | Mo | Cu | Nb+Ta | |
GB/T TULAFONO | 0.15 | 1.0-4.5 | 0.80 | 12.00 | 12.0-17.0 | ≥55 | 2.5-5.5 | 0.50 | 0.5-3.0 | |
TULAFONO AWS | 0.15 | 1.0-4.5 | 0.75 | 12.00 | 12.0-17.0 | ≥55 | 2.5-5.5 | 0.50 | 0.5-3.0 | |
FA'ATA'ITA'I TAUA | 0.07 | 2.6 | 0.28 | 4.03 | 14.3 | 66.6 | 4.41 | 0.060 | 1.67 |
MESINO MESIN:
MEATOAGA | MALOSI ALO'O (MPa) | MALOSI FA'ATA'U(MPa) | TULAGA TAUA J/℃ | ELONGATION(%) | ||||
GB/T TULAFONO | 360 | 650 | - | 18 | ||||
TULAFONO AWS | - | 650 | - | 25 | ||||
FA'ATA'ITA'I TAUA | 460 | 680 | - | 41.5 |
FAUTUAGA FA'ATAUUILOGA:
TITAMI FA'ĀMATALAGA (mm) | 2.6*300 | 3.2*350 | 4.0*350 | ||||||||
ELESI (Amp) | H/W | 69-95 | 70-115 | 95-145 | |||||||
O/W | 55-80 | 65-110 | 80-130 |
Low hydrogen type lima electrode, nominal composition (pasene i le mamafa) o le Ni14Cr4FeNbMo, nickel - chromium - uʻamea uʻamea electrode.
Stable arc, matagofie le fausiaina, laʻititi laʻititi, faigofie le aveeseina o le slag.
Lelei porosity teteʻe, o mea faʻainisinia o uʻamea uʻamea e mautu.
-
Nanjing Chengzhi Yongqing Malosiaga 07MnNiMoDR uamea ethylene polo tane
Reactor totonu
-
Arctic LNG-2 poloketi
VAEGA KEMIMI:
ALOY(wt%) | C | Mn | Si | Fe | Cr | Ni | Mo | Cu | Nb+Ta | |
GB/T TULAFONO | 0.15 | 1.0-4.5 | 0.80 | 12.00 | 12.0-17.0 | ≥55 | 2.5-5.5 | 0.50 | 0.5-3.0 | |
TULAFONO AWS | 0.15 | 1.0-4.5 | 0.75 | 12.00 | 12.0-17.0 | ≥55 | 2.5-5.5 | 0.50 | 0.5-3.0 | |
FA'ATA'ITA'I TAUA | 0.07 | 2.6 | 0.28 | 4.03 | 14.3 | 66.6 | 4.41 | 0.060 | 1.67 |
MESINO MESIN:
MEATOAGA | MALOSI ALO'O (MPa) | MALOSI FA'ATA'U(MPa) | TULAGA TAUA J/℃ | ELONGATION(%) | ||||
GB/T TULAFONO | 360 | 650 | - | 18 | ||||
TULAFONO AWS | - | 650 | - | 25 | ||||
FA'ATA'ITA'I TAUA | 460 | 680 | - | 41.5 |
FAUTUAGA FA'ATAUUILOGA:
TITAMI FA'ĀMATALAGA (mm) | 2.6*300 | 3.2*350 | 4.0*350 | ||||||||
ELESI (Amp) | H/W | 69-95 | 70-115 | 95-145 | |||||||
O/W | 55-80 | 65-110 | 80-130 |